Photolam De-lamination
Photolam cloth lamination. (Type – I) Photolam –PCL 120
This is a traditional method called chiffon lamination. In this process we have changed the material alone. Instead of natural chiffon cloth we are using cotton blended synthetic polyester meshed cloth and instead of starch paste we are using Poly vinyl Alcohol (PVOH) & Corboxy methyl cellulose (Sodium) [CMC (Na) ] mixed adhesive this is a water soluble adhesive .



Photolam tissue-lamination Method:
This is standardized in British Standard, which is adapted in India. This method is called tissue- lamination. In this process we are using Tissue paper (Extract - Banana leaf) of thickness 9-12GSM as reinforcement and paste as starch or CMC. We are using Poly vinyl Alcohol (PVOH) & Carboxyl methyl cellulose (Sodium) [CMC (Na) ] mixed in 1:10 ratio and then by dissolving them in 2% alcoholic distilled water and adhesive is prepared This is a reversible process and delaminating is possible with steam, sprit, or water. 


In cloth &tissue method, adhesive is prepared as follows:
50 gms of PVOH in 1000 ml. of lukewarm distilled water in a jar stirred well until dissolved. Then 50 gms of CMC(Na) is to be dissolved in another 1000ml of lukewarm distilled water in separate jar stirred well and close the top of the jars. Leave these two jars for an hour to settle, and then mix the two solutions in a big single jar. Leave them for twelve hours to settle; now we got our adhesive. This adhesive should used within 48 to 72 hours.